Corrosion experiments were conducted to provide insight into the nature of corrosion on the deep ocean floor. Corrosion rates were determined for carbon steel, low alloy steel, carbon steel in contact with stainless steel, Ni-Cr-Fe alloy 600, and various stainless steels in deep ocean environments. Specimens for corrosion studies were deployed mostly by submersible at depths between 3000 and 3700 meters for exposure periods of up to seven years. Experimental conditions for determining corrosion behavior were flowing, stagnant, and semi-stagnant seawater. Specimens were also completely buried in sediment and buried in sediment with the addition of a steel cover plate to blanket the sediment surface. Mean long term rates as shown in the following graph ranged from .03 to 2.75 mils per year for carbon steel (CS-516) and low alloy steel (HY-80) and up to 8.49 mils per year for carbon steel in contact with stainless steel (galvanic effect). Specimens buried in the sediment demonstrated the largest variability with individual specimen corrosion rates for carbon steel as great as 6.5 mils per year. When a steel plate covered the sediment the corrosion rate decreased to a relatively constant rate of .15 mils per year. Experiments were conducted in shallow watermore » sites for corrosion rate comparisons with deep water exposures. Shallow water experiments generally produced rates ten times higher for specimens submerged in the sediment and thirty percent higher in flowing environments. Several Atlantic and Pacific Ocean sites were also used for comparison studies and results showed moderate differences. 9 refs., 10 figs., 8 tabs.« less