The superabsorbent resin was synthesized from carboxymethyl cellulose and acrylic acid by aqueous solution polymerization.The optimal synthetic conditions were found as follows: acrylic acid 18 g,carboxymethyl cellulose 2 g,NaOH 7.2 g,deionized water 50 g,K2S2O8 0.5 g,N,N’-methylene bisacrylamide solution(1 g/L) 3 mL,polymerization temperature 60℃,time 1.5 h,and vacuum drying temperature 60℃.This resin could absorb 474.2 times its own mass in deionized water.The absorbencies of this superabsorbent in deionized water,tap water,artificial urine,artificial blood and normal saline were examined respectively.The water-absorbing rate,water-keeping function and reproducibility of the resin were also tested.