Ultrafine silver powder was prepared by liquid-phase reduction method using dilute sulphuric acid as dispersant,ascorbic acid as reducing agent and silver nitrate as metal source.Effects of reactant mixing manner,silver nitrate concentration and temperature on the characteristics of silver particles were studied. Properties of the silver powder was characterized by laser particle analyzer,scanning electron microscopy,x-ray diffraction and tapping apparatus.Optimum condition was:[AgNO3]=0.5mol/L;n(C6H8O6)∶n(AgNO3)= 2∶1;mass ratio of dispersant to silver nitrate=10%;pH=5;reactant mixing by dumping the reducing agent quickly into the silver nitrate solution;and reaction at room temperature.Monodisperse spherical silver particles with mean particle size of 2.5μm,apparent density of 2.5g/cm3 and tap density of 4.6g/cm3 can be obtained at the optimum condition.