The creep deformation in 72wt%Al2O3-mullite (72A), 74wt%Al2O3-mullite (74A) and those containing 10vol%ZrO2 (72A-10Z and 74A-10Z, respectively) has been studied. Stress exponent n's for creep in 72A-10Z and 74A-10Z were 1.1-1.2 and 1.0-1.2, respectively, slightly smaller than those in 72A (1.2-1.3) and 74A (1.3-1.5). Activation energies for creep in 72A-10Z and 74A-10Z were 157 and 158kcal/mol, respectively, slightly smaller than those in 72A and 74A (171 and 169kcal/mol, respectively). Creep rate in 74A was increased more than that in 72A by addition of 10vol% ZrO2. It was estimated that the enhanced creep rate of mullite ceramics by the addition of ZrO2 was ascribed to the relaxation of the stress at grain boundary triple points by the creep deformation of ZrO2 grains.