Nano-powders of 1.5TiAl and Al2O3 were synthesized from 1.5TiO2 and 3Al powders by high energy ball milling. Nanocrystalline Al2O3 reinforced composite was consolidated by pulsed current activated sintering within 2 minutes from mechanochemically synthesized powders of Al2O3 and 1.5TiAl. The relative density of the composite was 99.5%. The average hardness and fracture toughness values obtained were 1250 kg/mm and 10 MPa ·m, respectively. (Received September 5, 2011)