Orthogonal experiment method was used to investigate the effects of NiSO4·6H2O 、NaH2PO2·H2O、C3H6O2、H3BO3、pH and temperature on electroless Ni-P plating on quartz optical fiber surface when the combination extent between Ni-P thin film and fiber surface and Ni-P deposition rate were taken as the two objuctive functions.The optimal values of the six factors above were determined as: 35 g·L-1,32 g·L-1,20 mL·L-1,28 g·L-1,pH 5 and 84 ℃,respectively.The effect of coarsening time on film quarlity was also studied.SEM,SM,ICP and XRD were used to characterize and analyze the morphology,composition and structure of Ni-P film,respectively.The results showed that the Ni-P film deposited under the selected pretreatment conditions and the optimal electroless plating conditions has qualified properties with smoother and lucent surface,good combining force and without falling off after thermal shock test.