Abstract In this paper, a new type of AlSiMgCuNiAg filler metal was developed. The solidus temperature of the filler metal is 509.1°C and the liquidus temperature is 531.3°C. The filler metal has a good wetting and spreading effect on the surface of 6061 aluminum alloy. The CuAl2 phase in the brazing seam was greatly aggregated after brazed, while the CuAl2 phase was reduced and Mg2Si strengthening phase was formed when the brazed joints with heat treatment. The average shear strength of the brazed joint without heat treatment was 47.1MPa, and the average shear strength of the brazed joint with heat treatment reached to 108.7Mpa. The strength of the brazed joint with heat treatment was increased by about 131% relative to the strength of the brazed joint without heat treatment.