材料科学
复合数
陶瓷
复合材料
化学工程
工程类
作者
Li Ma,Jincheng Yu,Xue Guo,Yujun Zhang,Hongyu Gong
出处
期刊:Micro & Nano Letters
[Institution of Engineering and Technology]
日期:2018-04-05
卷期号:13 (7): 947-950
被引量:55
标识
DOI:10.1049/mnl.2017.0709
摘要
Titanium diboride–boron carbide (TiB 2 –B 4 C) composite ceramics were prepared using different amounts of Ni as sintering aids by pressureless sintering at 2100°C for 60 min under an argon atmosphere. This study focused on the effects of different amounts of Ni as additives on densification and mechanical and thermal properties of TiB 2 –B 4 C composite ceramics. Results showed that the relative density, hardness, flexural strength and thermal conductivity of obtained composite ceramics with 1.3 wt% Ni addition were 98%, 20.4 GPa, 330 MPa and 30 W/m K, respectively. However, fracture toughness was 6 MPa m 1/2 when the content of Ni was fixed at 2.2 wt%.