摘要
Silicon (Si) has attracted much attention as an emerging negative electrode material for all-solid-state lithium-ion batteries (ASSLIBs) because of the considerably high theoretical energy-density. However, its notorious volume changes during charge/discharge cycles often cause the rapid capacity fading. Thus, investigations into physicochemical and mechanical phenomena in Si electrodes during electrochemical lithiation/delithiation under ASSLIB configurations are of great importance. Single-crystal Si ( sc -Si) is an excellent subject of research to understand the anisotropic lithiation/delithiation characteristics by using different face orientations. Nevertheless, the available studies to date are mainly focused on the conventional-type LIB systems, which employ liquid organic-compounds as the main electrolyte components 1,2 . We have previously revealed the nanomechanical phenomena in a thin-film amorphous Si ( a -Si) electrode assembled in an ASSLIB configuration during the first electrochemical lithiation/delithiation using our newly constructed operando bimodal atomic force microscopy (AFM) system for solid-state batteries 3 . A steep elastic modulus decrease was observed at the initial stage of the lithiation, due to the formation of lithium silicide (Li x Si), followed by a gradual modulus reduction up to the completion of the first lithiation 3 . Likewise, operando X-ray photoelectron spectroscopy (XPS) analysis of the a -Si electrode indicated a steep binding energy shift of the bulk Si 0 peak to form Li x Si in the initial stage of lithiation, followed by the monotonic shift in response to the increase of Li content x in Li x Si 4-6 . Interestingly, a drastic peak shift associated with the phase transformation from crystalline Li 15 Si 4 ( c -Li 15 Si 4 ) into a -Li x Si was detected at Li content x = 1.6 – 2.0 in Li x Si during the subsequent delithiation, which caused the significant capacity loss probably due to the mechanical phenomena 4-6 . Electrochemical lithiation of sc -Si electrodes is known to be anisotropic 1,2 , and thus, a guideline to mitigate the rapid capacity fading due to the mechanical phenomena can be obtained by understanding the lithiation/delithiation mechanism of sc -Si electrodes, leading to the development of the long-lived Si-based negative electrode materials. In this study, we investigate the anisotropic electrochemical lithiation behaviors in sc -Si electrodes with different surfaces of (110), (100), and (111), evaluated using a variety of techniques including transmission electron microscopy (TEM), scanning electron microscopy (SEM), and XPS. ASSLIB half-cells with a configuration of sc -Si working electrode/lithium phosphorous oxynitride (LiPON) solid-electrolyte/Li metal counter electrode ( sc -Si/LiPON/Li) were fabricated from commercially available sc -Si wafers by sputter-deposition of a LiPON layer, followed by incorporation of a piece of Li metal foil. After the electrochemical lithiation, the sc -Si/LiPON/Li cells were cleaved to expose their cross-sections in an inert Ar-filled glove box, transported via a sealed transfer vessel, and analyzed by the above-mentioned techniques. At all the surface orientations (110), (100) and (111), the formation of a -Li x Si layer was clearly observed between the LiPON layer and sc -Si electrode. However, the Li content x in a -Li x Si layer was significantly different depending on the surface orientations, confirming the anisotropic lithiation reaction and Li-ion diffusion. The details including chemical species and nanomechanical properties will be discussed at the meeting as well as the anisotropic reaction mechanism. References (1) Aoki, N.; Omachi, A.; Uosaki, K.; Kondo, T., ChemElectroChem 2016, 3 (6), 959. (2) Omachi, A.; Aoki, N.; Uosaki, K.; Kondo, T., ECS Trans. 2017, 75 (52), 67. (3) Putra, R. P.; Matsushita, K.; Ohnishi, T.; Masuda, T., J. Phys. Chem. Lett. 2024, 15 (2), 490. (4) Endo, R.; Ohnishi, T.; Takada, K.; Masuda, T., J. Phys. Chem. Lett. 2020, 11 (16), 6649. (5) Endo, R.; Ohnishi, T.; Takada, K.; Masuda, T., J. Phys. Commun. 2021, 5 (1), 015001. (6) Endo, R.; Ohnishi, T.; Takada, K.; Masuda, T., J. Phys. Chem. Lett. 2022, 13 (31), 7363.